180 Degree Peel Test Procedure and Specimen Preparation

By Lim Xu, Export Manager

A 180 degree peel test pulls a flexible strip back over itself and measures the force needed to separate it from its bonded surface. Labs use it for pressure-sensitive tapes, self-adhesive labels and flexible-to-rigid bonded assemblies. This guide covers the main standards, specimen preparation, the test run and how 180 degree peel differs from 90 degree peel.

What a 180 degree peel test measures

The test measures peel resistance, the force that keeps a bond together as it is opened along its length. ASTM D903 calls this peel or stripping strength and uses a separation angle of approximately 180 degrees. At least one of the bonded materials must be flexible enough to turn back at that angle.

In ISO 8510-2 the two parts are pulled apart at a steady rate, starting from the open end of the bond. Separation moves progressively along the bond, and the force acts through the peeled part of the flexible strip.

For pressure-sensitive tape, ASTM D3330 Method A peels a single-coated tape at 180 degrees from a standard steel panel or another surface of interest. The standard presents this as a check of adhesion uniformity within a roll, between rolls or between production lots.

Standards that use a 180 degree peel

Several methods use the same angle but different specimens. The table lists four of these methods.

StandardWhat it coversRelated 90 degree method
ASTM D903Peel or stripping strength of adhesive bonds, with at least one flexible adherendn/a
ASTM D3330/D3330M Method ASingle-coated pressure-sensitive tape on a steel panel or other surfaceMethod F in the same standard
ISO 8510-2Adhesive bond between a flexible adherend and a rigid adherendISO 8510-1
FINAT FTM 1Peel adhesion (180 degree) at 300 mm/min, from the FINAT label industry test methodsFINAT FTM 2

Peeling a heat seal is a different job. Seal strength of flexible packages is measured under ASTM F88, as our guide to flexible packaging testing equipment explains.

Questions about a model or a test? Email Amy Zhao, Export Manager, at [email protected].

Preparing and conditioning specimens

ISO 8510-2 gives a clear example of specimen preparation for a flexible strip bonded to a rigid strip. Follow the method your own specification names, since tape and label methods use their own panels and strips.

  1. Cut the rigid strip 25.0 ± 0.5 mm wide and at least 200 mm long.
  2. Cut the flexible strip at least 350 mm long and the same width, or 5 mm wider at each edge if it frays.
  3. Apply adhesive across the full width over 150 mm, with an anti-adhesive strip at the start of the bond.
  4. Bond with even pressure, then set or cure the adhesive as its maker instructs.
  5. Prepare at least five specimens.

Condition and test the specimens in one of the standard atmospheres of ISO 291. Measure the adherends and the adhesive thickness, because both go into the test report.

Stiff backings need care. ASTM D3330 warns that tapes with stiff backings or liners, or backings that stretch at low force, give highly variable results.

Running the test and reading the curve

Bend back the unbonded end of the flexible strip. Clamp the rigid strip in the fixed grip and the flexible strip in the self-aligning grip. The tension should spread evenly across the specimen width.

ISO 8510-2 recommends a grip separation rate of 100 ± 10 mm/min and continues until at least 125 mm of bond has separated. FINAT FTM 1 runs at 300 mm/min, so always use the rate your method sets. Note whether each specimen shows adhesive failure, cohesive failure or failure of the adherend itself.

From the force against grip separation curve, take the average peel force over at least 100 mm, leaving out the first 25 mm. Record the maximum and minimum in that range, then average all specimens. Initial peaks outside the measured length may be recorded separately but stay out of the average.

The testing machine matters too. ISO 8510-2 asks for indicated force within 2% of the true force. It also asks for a force at rupture between 10% and 80% of the full-scale reading.

Our WDB-01 180 degree peel tester lists a 180 degree tape peel test as its test method. Tell us which method your customer specifies and our factory team can reply by email.

90 degree vs 180 degree peel

ISO 8510-1 describes a 90 degree peel for less flexible adherends that crack, break or delaminate in the 180 degree test. ASTM D3330 Method F and FINAT FTM 2 are the 90 degree versions of their 180 degree methods.

Results at the two angles are separate methods, so do not mix them in one data set. Report the angle and the grip separation rate with every peel result.

In a 180 degree test, the peeled part rubs on the bonded part as the test goes on. ISO 8510-2 allows a lubricant such as glycerol or soap solution to cut this friction, if it does not affect the adherends.

Frequently asked questions

Can I compare peel results for tapes from two different makers?

Not directly with most ASTM D3330 methods. The standard says Methods A, B, C, E and F cannot compare two tapes of the same type from different makers. The reason is that the peel force is not normalized for a fixed stressed area.

Does a peel test value tell me how a tape will perform in use?

Not usually. ASTM D3330 states that its methods may not provide design information, since there is usually no direct link between peel adhesion and a functional requirement. Use peel values for quality control against an agreed minimum or maximum.

Talk to our factory team

We sell direct from our factory, so you work directly with our factory team. Questions about a model or a test? Email Amy Zhao, Export Manager, at [email protected].

Related articles

Let's Talk

We're here to help you with your needs. Let's talk about how we can help you.

View our privacy policy.

© 2026 KHT Instruments | All rights reserved.