Tensile Strength of Paper and How to Test It under ISO 1924
By Lim Xu, Export Manager
The tensile strength of paper is the maximum tensile force per unit width that a strip withstands before it breaks. It is usually reported in kN/m. ISO 1924-2 and TAPPI T 494 measure it by pulling a strip at a constant rate of elongation.
What tensile strength of paper means
Because the result is force divided by strip width, paper tensile strength is not a stress like the MPa values used for plastics. Thickness is needed only if you also calculate the modulus of elasticity.
ISO 1924-2 always includes tensile strength. Strain at break, tensile energy absorption and the modulus of elasticity are measured only when the parties agree to it. TAPPI T 494 covers four breaking properties: tensile strength, stretch, tensile energy absorption and tensile stiffness.
Tensile strength is used to judge how well paper resists a web break. It matters for printing, converting and packaging papers.
Paper tensile units in kN/m, tensile index and breaking length
Tensile strength is expressed as force per unit width, usually kN/m. Some reports give it in lbf/in or kgf per 15 mm strip, and the table below shows how to convert them.
| Quantity | Other unit | Multiply by | SI unit |
|---|---|---|---|
| Tensile strength | lbf/in | 0.175127 | kN/m |
| Tensile strength | kgf/15 mm | 0.65378 | kN/m |
| Tensile index | km breaking length | 9.80665 | N·m/g |
Tensile index is tensile strength divided by grammage. With tensile strength in kN/m and grammage in g/m², tensile index in N·m/g is 1,000 × tensile strength ÷ grammage.
Here is a hypothetical example with a tensile strength of 6.0 kN/m and a grammage of 80 g/m². The tensile index is 1,000 × 6.0 ÷ 80 = 75 N·m/g.
Breaking length is the older form of the same ratio, and tensile index has replaced it. Divide 75 N·m/g by 9.80665 to get a breaking length of about 7.65 km.
Bursting strength is a different paper property, measured as a pressure; our bursting strength unit guide covers its units.
Questions about a model or a test? Email Amy Zhao, Export Manager, at [email protected].
ISO 1924-2 and TAPPI T 494 test setup
ISO 1924-2 uses test pieces 15 mm ± 0.1 mm wide. The test length between the clamping lines is 180 mm ± 1 mm. The clamps separate at 20 mm/min ± 5 mm/min.
Each clamp grips the strip along a straight line across its full width, firmly but without slipping or damaging it. The machine must indicate force within ±1% of the true force.
ISO 1924-3 is the faster method, at 100 mm/min over a 100 mm span. ISO 1924-2 notes that in most cases tensile properties can rise by 5% to 15% at the faster setting. The two methods do not give the same values.
Condition the paper as set out in ISO 187 and test it in the same atmosphere. TAPPI T 494 also uses constant rate of elongation equipment; take its settings from the full method. Our WDK-01 paper tensile strength tester is listed on this site for paper tensile testing. Ask us which methods it is set up for.
MD and CD results
Paper fibres line up with the direction the web runs on the paper machine. Tensile strength is therefore higher in the machine direction (MD) than in the cross direction (CD), and both are usually measured.
ISO 1924-2 asks for at least ten valid results for each direction you test. Report MD and CD as separate averages rather than one combined value.
Reject any strip that breaks within 10 mm of a clamping line. If more than 20% of strips from one sample break there, check the machine against the standard before you trust the results. State the number of clamp breaks in the report.
Our paper models are listed in the tensile testers for film and paper collection.
What lowers paper tensile results
Some causes sit in the paper itself. Fibre strength, fibre length, fibre bonding, the degree of refining and fibre direction are the main sources of tensile strength, and fillers also affect it.
Other causes come from the test. ISO 1924-2 points to these:
- Moisture changes, since the test is very sensitive to the moisture content of the strip
- Bare hands touching the part of the strip that goes between the clamps
- Ragged or uneven edges; the long edges must be straight, parallel and cleanly cut
- Watermarks, folds or wrinkles in the test area
- Clamp slip or damage at the clamping line
A drop in results from one batch to the next is worth checking against these test causes before it is blamed on the paper.
Frequently asked questions
Can ISO 1924-2 be used on corrugated board?
Not on the finished board. ISO 1924-2 covers the component papers of corrugated board, but not the combined board itself. Test the component papers instead.
Can I use a shorter test length than 180 mm?
Yes, in some cases. ISO 1924-2 allows a smaller test length for high stretch paper or small samples. The rate of elongation should then be about 10% of the test length per minute, and both values should be stated in the test report.
Is tissue paper tested the same way?
No. ISO 1924-2 does not cover tissue paper and tissue products. ISO 12625-4 applies to them instead.
Talk to our factory team
We sell direct from our factory, so you work directly with our factory team. Questions about a model or a test? Email Amy Zhao, Export Manager, at [email protected].
Related articles
- Pouch Burst Test for Flexible and Medical PackagingA pouch burst test inflates a sealed package until it fails. Compare ASTM F1140 and F2054, burst and creep tests, and how to read where the pouch opened.
- Box Compression Test Standards ASTM D642 ISO 12048 and TAPPI T 804Compare the main box compression test standards, ASTM D642, ISO 12048 and TAPPI T 804, by scope, contents, orientation, speed and what to report.
- Bursting Strength Tester HS Code by CountryHow a bursting strength tester moves from HS subheading 9024.80 to national tariff lines, how binding rulings work, and what paperwork customs needs.
- Bursting Strength Tester Calibration and What Foils Can CheckBursting strength tester calibration under ISO 2758 and ISO 2759 covers pumping rate, peak pressure and clamping. See why foils check function only.